Technical Article · Coating Analysis

Strontium in a Dicronite® Coating? Why EDX and XRF Can Give a False Positive

A customer's lab reported strontium on a part coated with Dicronite® DL-5®. Here is why X-ray analysis of a 0.5 µm film can name an element that is not there.

Dicronite Southwest 6 min read Based on LSI Technical Bulletin 121525

Interactive graphic

What the Instrument Actually Measures

Switch the analysis method or the spectrum view, or select a numbered point or a card to see the details.

Coating & Substrate · Interaction Volume

Analysis method

EDX spectrum, 1.1 to 2.1 keV

Illustration of the energies in the bulletin, not measured data. Mg and Cr are shown for scale, as in the bulletin.

Tap a number or swipe to see the next point.

The question

Strontium Detected in the Coating?

A customer ran analyses on parts coated with Dicronite® DL-5® and detected strontium in the coating. They asked whether strontium is expected in the coating, or whether it pointed to contamination.

The answer is neither. The strontium reading is a false positive, an artifact of the limits of X-ray analysis on a coating this thin. This article explains why, based on Lubrication Sciences International's Technical Bulletin 121525.

The analysis was most likely carried out with an industry-standard X-ray technique such as EDX or XRF. These methods are widely used and can be extremely valuable, but this case shows the fundamental limits they face on micron and sub-micron coatings deposited on a metal substrate.

Reason 1

X-Ray Methods See Through a 0.5 µm Coating

Dicronite® is deposited at about 0.5 µm thick. At that thickness, conventional X-ray techniques cannot analyze the coating on its own. The X-rays pass through the coating into the substrate below, so the result is a combined, proportional analysis of the coating and the base material, not the coating chemistry alone.

  • SEM-EDS / EDX

    Energy-dispersive X-ray spectroscopy. Readily detects tungsten and sulfur in the coating, but reaches well past it.

    ~1–3 µm deep
  • XRF

    X-ray fluorescence. Reaches much deeper into the part than EDX.

    ~5–50 µm deep
  • XPS

    X-ray photoelectron spectroscopy. Surface-sensitive, so it can characterize the coating without interference from the substrate.

    Nanometers deep
  • AES

    Auger electron spectroscopy. Also surface-sensitive, probing only the top nanometers of the part.

    Nanometers deep
10–20%At an analysis depth of 2.5 to 5 µm, the 0.5 µm coating makes up only about 10–20% of the volume analyzed. The substrate makes up about 80–90% of the result.

Any element detected this way on a 0.5 µm Dicronite® coating is strongly influenced, if not dominated, by the substrate and any contamination near the surface. Strontium found this way cannot automatically be attributed to the coating.

Reason 2

Three Peaks Closer Than the Detector Can Separate

In this case the substrate contained no strontium either. The rest of the answer lies in how close together the X-ray energies of tungsten, silicon and strontium are.

  • 1.739 keVSi KαSilicon, from the substrate
  • 1.775 keVW MαTungsten, from the coating
  • 1.806 keVSr LαStrontium, not present in the part
30–40 eVThe gap between these adjacent peaks, smaller than the typical resolution of a standard EDX detector, about 120–140 eV.

What happens during EDX analysis

  1. Tungsten (W) from the coating is detected, as expected.
  2. Silicon (Si) from the substrate is detected at the same time, because the interaction volume extends through the coating into the substrate.
  3. The W and Si signals partly overlap in the low-energy region, and the analysis software tries to separate them.
  4. Because of software limits, the combined signal is assigned to strontium, the nearest element in this closely spaced group, even though no strontium is present.

The result is a best-fit false positive, a known artifact of standard EDX systems.

An analogy

Green, Blue and a Color That Is Not There

Think of the tungsten signal as a green peak and the silicon signal as a blue peak. Because the two peaks are so close together, the detector sees a blend of green and blue. The software, trying to name that blend, matches it to the closest color in its library, the one that stands for strontium. The result is a false positive, even though no strontium is present in the substrate or the coating.

The right test

Analyzing a Thin Film Accurately

Accurate elemental analysis of a coating about 0.5 µm thick needs a surface-sensitive technique, such as X-ray photoelectron spectroscopy (XPS) or Auger electron spectroscopy (AES). These probe depths on the nanometer scale and can characterize the coating without interference from the substrate.

Bulk techniques such as EDS/EDX and XRF are inherently influenced by the substrate, which can lead to false positives, exactly as in this case.

  • XPS
  • AES
  • Nanometer-scale depth
  • No substrate interference

Quality assurance

Why We Are Confident Dicronite® Contains No Strontium

  • Dicronite® raw powder undergoes chemical analysis every quarter
  • The coating is tested, approved and certified to the latest AMS 2530 aerospace specification for tungsten disulfide films
  • The strontium reading is explained by the limits of the X-ray analysis equipment

The outcome

The Customer's Response

The customer thanked the team for confirming there was no strontium in the coating. They had suspected as much from their SEM results and wanted confirmation, and found that the explanation matched the results they had seen.

Summary

A False Positive, Not Contamination

On a 0.5 µm Dicronite® coating, EDX and XRF mostly measure the substrate. Silicon from the substrate and tungsten from the coating produce peaks only 30–40 eV apart, closer than a standard EDX detector can resolve, and the software's best fit can name strontium even though none is present.

With quarterly analysis of the raw powder and certification to AMS 2530, Dicronite® is strontium-free. To analyze the coating itself, use a surface-sensitive method such as XPS or AES.

Questions About Testing a Coated Part?

Tell us what analysis you ran and what it showed, and our team will help you interpret the results for your Dicronite® coated parts.

Dicronite® Southwest

Request a Dicronite® WS₂ Coating Quote

Send us your project details so we can evaluate your requirements and prepare a quote.

Sending drawings securely

Dicronite® Southwest is CMMC compliant. Please do not attach drawings to this form. Send drawings, including ITAR and CUI technical data, by email to rfq@secure.dicronitesouthwest.com. Email to this secure address is routed into our PreVeil encrypted environment.

Submit this form first so our team can add your email address, or your company's email domain, to the approved list for the secure inbox. Email from addresses that are not on the list cannot be received.

If your company already uses PreVeil, you can also send drawings to us directly through PreVeil.

Email Drawings Securely

Loading the quote form…

Thank you. Your quote request has been received.

Our team will review your project details and follow up by email.